{"id":838,"date":"2026-10-14T05:29:00","date_gmt":"2026-10-14T05:29:00","guid":{"rendered":"https:\/\/academicsociety.org\/bio\/?p=838"},"modified":"2026-11-24T06:15:09","modified_gmt":"2026-11-24T06:15:09","slug":"green-synthesis-of-copper-oxide-cuo-nanoparticles-using-tulsi-ocimum-sanctum-leaf-extract-structural-characterization-antioxidant-activity-and-antibacterial-activity-against-escherichia-coli","status":"publish","type":"post","link":"https:\/\/academicsociety.org\/bio\/2026\/10\/14\/green-synthesis-of-copper-oxide-cuo-nanoparticles-using-tulsi-ocimum-sanctum-leaf-extract-structural-characterization-antioxidant-activity-and-antibacterial-activity-against-escherichia-coli\/","title":{"rendered":"Green Synthesis of Copper Oxide (CuO) Nanoparticles Using Tulsi (Ocimum sanctum) Leaf Extract: Structural Characterization, Antioxidant Activity and Antibacterial Activity against Escherichia coli"},"content":{"rendered":"\n<h1 class=\"wp-block-heading\">Introduction<\/h1>\n\n\n\n<p>Metal oxide nanoparticles have attracted wide interest because their small size and large surface-to-volume ratio give them optical, catalytic and biological properties that differ from those of the bulk material. Among them, copper oxide (CuO) is a p-type semiconductor with a narrow band gap, and it is inexpensive and relatively easy to prepare [1,2]. CuO nanoparticles have been explored for antimicrobial, antioxidant, catalytic and sensing applications [2,3]. Conventional physical and chemical routes to nanoparticles often need high energy input, toxic reagents or hazardous by-products. Green synthesis, in which plant extracts act as reducing and stabilizing agents, offers a simpler, cleaner and more economical alternative [2,4]. Plant extracts are rich in polyphenols, flavonoids, terpenoids, proteins and sugars, which can reduce metal ions and cap the growing particles, limiting uncontrolled growth and providing surface functional groups that may contribute to biological activity.<\/p>\n\n\n\n<p>Tulsi (<em>Ocimum sanctum<\/em>, holy basil) is widely available in India and has a long history of use in traditional medicine. Its leaves contain phenolic compounds and flavonoids, which makes the extract a suitable candidate for nanoparticle synthesis [5]. Because resistant bacteria and oxidative stress-related disorders remain major health concerns, nanomaterials that show both antioxidant and antibacterial behaviour are of practical interest. <em>Escherichia coli<\/em> is a common Gram-negative test organism for such work. In this work, CuO nanoparticles were synthesized using Tulsi leaf extract and characterized by XRD, FTIR, SEM and EDAX. Their antioxidant activity was assessed by the DPPH radical scavenging assay, and their antibacterial activity against <em>E. coli<\/em> was evaluated by the agar well-diffusion method.<\/p>\n\n\n\n<h1 class=\"wp-block-heading\">2. Materials and Methods<\/h1>\n\n\n\n<h2 class=\"wp-block-heading\">2.1 Preparation of Tulsi leaf extract<\/h2>\n\n\n\n<p>Fresh Tulsi (<em>Ocimum sanctum<\/em>) leaves were collected from local area, washed thoroughly with distilled water and dried. About 10 gm of leaves was boiled in 200 mL of distilled water at 40-50 \u00b0C for 2 hrs min, cooled and filtered through Whatman No. 1 filter paper. The filtrate was used as the reducing and capping agent.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">2.2 Green synthesis of CuO nanoparticles<\/h2>\n\n\n\n<p>Copper precursor, e.g. copper sulphate pentahydrate merk&nbsp; was mixed with 640mL of Tulsi leaf extract under stirring at 50-60 \u00b0C] for 3 hrs min. &nbsp;a colour change was observed. The precipitate was collected by centrifugation, washed with distilled water and ethanol, dried at 80\u00b0C at oven and calcined at &nbsp;400 \u00b0C for&nbsp; 3hrs to obtain CuO nanoparticles.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">2.3 Characterization<\/h2>\n\n\n\n<p>The crystal structure was examined by powder XRD ,Cu K\u03b1 radiation, \u03bb = 1.54059 \u00c5) and compared with the reference tenorite CuO pattern (COD 9015822). The crystallite size (<em>D<\/em>) was calculated from the Debye\u2013Scherrer equation:<\/p>\n\n\n\n<p><em>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp; D = K\u03bb \/ (\u03b2 cos\u03b8)&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp; (1)<\/em><\/p>\n\n\n\n<p>where <em>K<\/em> = 0.9, \u03bb is the X-ray wavelength, \u03b2 is the full width at half maximum (FWHM) in radians and \u03b8 is the Bragg angle. To separate the contributions of crystallite size and lattice microstrain (\u03b5) to peak broadening, the Williamson\u2013Hall (uniform deformation model) relation was used:<\/p>\n\n\n\n<p><em>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp; \u03b2 cos\u03b8 = K\u03bb \/ D + 4\u03b5 sin\u03b8&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp; (2)<\/em><\/p>\n\n\n\n<p>The dislocation density (\u03b4) was estimated as:<\/p>\n\n\n\n<p><em>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp; \u03b4 = 1 \/ D\u00b2&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp; (3)<\/em><\/p>\n\n\n\n<p>Surface functional groups were identified by FTIR spectroscopy (Shimadzu) over 4000\u2013400 cm\u207b\u00b9 .The surface morphology was observed by SEM at \u00d7250 and \u00d710,000 magnification, and the elemental composition and distribution were determined by EDAX elemental mapping and eZAF quantification.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">2.4 Antioxidant activity (DPPH assay)<\/h2>\n\n\n\n<p>The free radical scavenging activity was determined by the DPPH (1,1-diphenyl-2-picrylhydrazyl) method [6,7]. In a 96-well plate, 10 \u00b5L of sample at different concentrations was added to 0.2 mL of 0.1 mM DPPH solution in methanol. Ascorbic acid was the positive standard (0\u201350 \u00b5g\/mL), and the nanoparticles were tested over 0\u20131000 \u00b5g\/mL. Reactions were run in quadruplicate with duplicate DPPH-free blanks. After 30 min of incubation in the dark, absorbance was read at 517 nm using a microplate reader (iMark, Bio-Rad). The percentage of radical scavenging activity (% RSA) was calculated as:<\/p>\n\n\n\n<p><em>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp; % RSA = [(Abs_control \u2212 Abs_sample) \/ Abs_control] \u00d7 100&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp; (4)<\/em><\/p>\n\n\n\n<p>and the IC\u2085\u2080 values were calculated with GraphPad Prism 6.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">2.5 Antibacterial activity (well-diffusion assay)<\/h2>\n\n\n\n<p>Antibacterial activity was evaluated against <em>Escherichia coli<\/em> (MTCC 452) by the agar well-diffusion (Kirby\u2013Bauer) method [8]. Mueller\u2013Hinton agar plates were inoculated with 100 \u00b5L of bacterial culture adjusted to 0.5 McFarland standard (~1.5 \u00d7 10\u2078 CFU\/mL). Wells &nbsp;were loaded with 50 \u00b5L of nanoparticle suspension at 0, 312.5, 625, 1250, 2500 and 5000 \u00b5g\/mL. One well on each plate received the solvent alone (DMSO, vehicle control) and one received ciprofloxacin (3 \u00b5g) as the positive control (PC). Plates were incubated at 37 \u00b0C for 24 h, and the clear zones were measured in mm. All nanoparticle plates were run in duplicate (Plate A and Plate B).<\/p>\n\n\n\n<h1 class=\"wp-block-heading\">3. Results and Discussion<\/h1>\n\n\n\n<h2 class=\"wp-block-heading\">3.1 XRD analysis<\/h2>\n\n\n\n<p>The XRD pattern of the Tulsi-mediated CuO sample was compared with the reference tenorite pattern (COD 9015822; monoclinic, space group C2\/c; <em>a<\/em> = 4.6776 \u00c5, <em>b<\/em> = 3.4593 \u00c5, <em>c<\/em> = 5.1264 \u00c5, \u03b2 = 98.965\u00b0). The strong reflections, the most intense of which were (11\u22121) at 35.18\u00b0 and (111) at 38.41\u00b0, all indexed to monoclinic CuO (Table 1), and no reflections from Cu\u2082O, Cu(OH)\u2082 or unreacted precursor were detected. A very weak reflection at 30.18\u00b0 (relative intensity 5.6) does not match any tenorite line. Given its low intensity it is most likely a trace impurity or residual phytochemical crystallite, and it could be checked against Cu(OH)\u2082 and basic copper carbonate references if full phase purity is to be claimed.<\/p>\n\n\n\n<p>The average crystallite size from the Debye\u2013Scherrer equation, using 14 reliable reflections, was about 33.0 nm (Fig. 1). The Williamson\u2013Hall plot (Fig. 2) had a positive slope, indicating a small lattice microstrain of about 2.3 \u00d7 10\u207b\u2074, and its intercept gave a crystallite size of about 54 nm. The dislocation density calculated from the Scherrer size was about 9.2 \u00d7 10\u00b9\u2074 lines\/m\u00b2. The difference between the two size estimates reflects the different assumptions of the methods, and it is therefore useful to report both values (Table 2).<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">3.2 FTIR analysis<\/h2>\n\n\n\n<p>The FTIR spectrum (Fig. 3, Table 3) was recorded to identify the functional groups on the nanoparticle surface and to confirm formation of the metal\u2013oxygen lattice. The broad, intense band at 3367.86 cm\u207b\u00b9 is assigned to O\u2013H stretching of adsorbed water and of phenolic and hydroxyl groups from the Tulsi phytoconstituents (e.g. flavonoids, tannins). The weak bands at 3960.99 and 3843.33 cm\u207b\u00b9 correspond to overtone\/combination bands and free surface hydroxyl stretching, and the weak bands between 2423.66 and 2040.77 cm\u207b\u00b9 are largely due to atmospheric CO\u2082 and combination modes. The band at 1627.99 cm\u207b\u00b9 is assigned to C=O stretching (amide I) and\/or aromatic C=C stretching, overlapping with the bending mode of adsorbed water. The bands at 1539.26 and 1390.74 cm\u207b\u00b9 correspond to N\u2013H bending\/aromatic C=C stretching (amide II) and to C\u2013N stretching\/symmetric carboxylate (COO\u207b) stretching, respectively, indicating residual proteins and phenolic biomolecules acting as capping and stabilizing agents. The bands at 1221.96 and 1072.47 cm\u207b\u00b9 are attributed to C\u2013O stretching of phenolic or ester groups and C\u2013O\u2013C stretching of polyol\/polysaccharide constituents. The bands at 914.30 and 792.78 cm\u207b\u00b9 are assigned to C\u2013H out-of-plane bending and Cu\u2013O\u2013H bending vibrations. Most diagnostically, the pair of bands at 603.75 and 512.12 cm\u207b\u00b9 is assigned to Cu\u2013O stretching of the monoclinic CuO lattice. The presence of these low-wavenumber bands, with no bands attributable to unreacted copper precursor, supports formation of the CuO phase, in agreement with the XRD result, while the O\u2013H, C=O, C\u2013N and C\u2013O bands confirm a biomolecule-derived organic layer on the particle surface.<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">3.3 SEM and EDAX analysis<\/h2>\n\n\n\n<p>At low magnification (\u00d7250, Fig. 4a) the CuO\u2013Tulsi sample appeared as highly agglomerated, porous clusters of irregular granular particles. Such agglomeration is common in plant-mediated synthesis, where capping biomolecules promote nucleation but also encourage secondary clustering during drying and calcination. At \u00d710,000 (Fig. 4b) the individual grains were angular and plate-like with sharp, well-defined edges, and fine particulates decorated the surfaces of the larger grains, suggesting nucleation of smaller CuO particles on larger secondary aggregates.<\/p>\n\n\n\n<p>EDAX elemental mapping (Fig. 5) showed copper and oxygen distributed across the imaged region, with copper-rich domains corresponding to the denser clusters and oxygen distributed fairly uniformly. The sum spectrum (Fig. 6) contained two dominant peaks, O K\u03b1 and Cu L\u03b1, with no peaks from other metallic contaminants. Quantification (Table 4, Fit A) gave 70.0 wt% Cu and 30.0 wt% O (37.0 at% Cu, 63.0 at% O). This is richer in oxygen than the ideal 1:1 Cu:O ratio of CuO (about 79.9 wt% Cu), which is often seen for green-synthesized oxides because oxygen-containing surface species (adsorbed water, hydroxyl and carboxylate groups of the capping layer) add to the oxygen signal and because EDAX is less accurate for light elements. The result therefore confirms a copper oxide with no foreign metals, and the CuO phase assignment rests mainly on the XRD and FTIR data.<\/p>\n\n\n\n<p>When adventitious carbon was included in the fit (Table 4, Fit B), the composition was 24.9 at% Cu, 48.7 at% O and 26.4 at% C. The carbon is attributed to residual phytochemical capping agents (flavonoids, terpenoids, phenolics) from the Tulsi extract, in line with the FTIR results, although carbon tape or a conductive coating can also contribute to this signal [9].<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">3.4 Antioxidant activity<\/h2>\n\n\n\n<p>The DPPH radical scavenging activity of CuO\u2013Tulsi increased with concentration, from 5.31% at 1 \u00b5g\/mL to 89.45% at 1000 \u00b5g\/mL, passing 50% between 100 \u00b5g\/mL (48.66%) and 250 \u00b5g\/mL (71.81%) (Table 5, Fig. 7a). Ascorbic acid, tested over the lower range of 0\u201350 \u00b5g\/mL, reached 84.20% at 50 \u00b5g\/mL (Fig. 7b). The IC\u2085\u2080 of CuO\u2013Tulsi was 102.9 \u00b1 0.02 \u00b5g\/mL compared with 19.97 \u00b1 0.02 \u00b5g\/mL for ascorbic acid, so the nanoparticles were about 5.15-fold less potent than the pure standard on a mass basis, which is expected for a purified antioxidant compound. The two series were measured over different concentration ranges, so percentage values at the same concentration should not be compared directly.<\/p>\n\n\n\n<p>In a screen of nine metal oxide\u2013plant combinations (FeO, NiO and CuO with Tulsi, Neem and Aloe vera extracts), CuO\u2013Tulsi was one of only three samples for which an IC\u2085\u2080 could be determined within 0\u20131000 \u00b5g\/mL, the others being NiO\u2013Neem (95.24 \u00b1 0.02 \u00b5g\/mL) and NiO\u2013Tulsi (140.3 \u00b1 0.02 \u00b5g\/mL). The remaining six samples did not reach 50% scavenging in this range. The activity of CuO\u2013Tulsi is likely due to residual phenolic and flavonoid compounds from the Tulsi extract adsorbed on the nanoparticle surface, which the FTIR and EDAX results support, although a contribution from the CuO itself cannot be ruled out. Antioxidant activity has also been reported for Cu and Ag nanoparticles prepared with <em>Ocimum sanctum<\/em> leaf extract [5].<\/p>\n\n\n\n<h2 class=\"wp-block-heading\">3.5 Antibacterial activity against E. coli<\/h2>\n\n\n\n<p>CuO\u2013Tulsi produced clear zones of inhibition against <em>E. coli<\/em> (MTCC 452) at all concentrations tested (Table 6, Fig. 8). The zone was 12 mm at every concentration from 312.5 to 5000 \u00b5g\/mL, with no variation between the duplicate plates, while the vehicle control (DMSO) produced no zone. The ciprofloxacin control (3 \u00b5g) gave a zone of 30.5 mm (SD 0.71).<\/p>\n\n\n\n<p>The unchanged zone size over a 16-fold concentration range suggests that the antibacterial effect saturates at or below the lowest concentration tested, probably because of limited diffusion of the nanoparticles through the agar. The minimum inhibitory concentration is therefore likely to lie below 312.5 \u00b5g\/mL, and it should be determined by a broth microdilution method. MIC values of 62.5\u2013125 \u00b5g\/mL against <em>E. coli<\/em> have been reported for CuO nanoparticles made with neem and jojoba extracts [9,11,13], which is below the lowest concentration used here. Compared with the other copper oxide samples prepared with different plant extracts (Table 7), CuO\u2013Tulsi was the only one to reach its full effect at the lowest concentration: CuO\u2013Aloevera reached similar zones only at 625\u20131250 \u00b5g\/mL, and CuO\u2013Neem reached a comparable zone (13 mm) only at 5000 \u00b5g\/mL. The antibacterial action of copper oxide nanoparticles is commonly attributed to release of Cu\u00b2\u207a ions, generation of reactive oxygen species and damage to the cell membrane [3,9,12]; these mechanisms were not examined in the present work, and the role of the Tulsi capping layer remains to be studied.<\/p>\n\n\n\n<h1 class=\"wp-block-heading\">4. Conclusion<\/h1>\n\n\n\n<p>CuO nanoparticles were synthesized using Tulsi (<em>Ocimum sanctum<\/em>) leaf extract. XRD showed single-phase monoclinic CuO with a crystallite size of about 33 nm (Debye\u2013Scherrer) or 54 nm (Williamson\u2013Hall) and a small microstrain of 2.3 \u00d7 10\u207b\u2074. FTIR confirmed Cu\u2013O lattice vibrations and a capping layer of plant biomolecules[10]. SEM showed agglomerated, faceted particles, and EDAX confirmed copper and oxygen with residual carbon from the extract. The nanoparticles scavenged DPPH radicals in a concentration-dependent manner (IC\u2085\u2080 = 102.9 \u00b1 0.02 \u00b5g\/mL) and produced a reproducible 12 mm inhibition zone against <em>E. coli<\/em> from 312.5 \u00b5g\/mL upwards. These findings indicate that Tulsi-mediated CuO nanoparticles are a promising antioxidant and antibacterial material. Further work should determine the MIC and MBC, test Gram-positive organisms, examine the mechanism of action and assess cytotoxicity.<\/p>\n\n\n\n<h1 class=\"wp-block-heading\">Conflict of Interest<\/h1>\n\n\n\n<p>The authors declare no conflict of interest.<\/p>\n\n\n\n<h1 class=\"wp-block-heading\">References<\/h1>\n\n\n\n<p>[1]&nbsp;&nbsp;&nbsp;&nbsp; Reddy, K. R. (2017). Green synthesis, morphological and optical studies of CuO nano-particles. <em>Journal of Molecular Structure<\/em>, 1150, 553\u2013557. https:\/\/doi.org\/10.1016\/j.molstruc.2017.09.005<\/p>\n\n\n\n<p>[2]&nbsp;&nbsp;&nbsp;&nbsp; Akintelu, S. A., Folorunso, A. S., Folorunso, F. A., &amp; Oyebamiji, A. K. (2020). Green synthesis of copper oxide nanoparticles for biomedical application and environmental remediation. <em>Heliyon<\/em>, 6, e04508.<\/p>\n\n\n\n<p>[3]&nbsp;&nbsp;&nbsp;&nbsp; Letchumanan, D., Sok, S. P., Ibrahim, S., Nagoor, N. H., &amp; Arshad, N. M. (2021). Plant-based biosynthesis of copper\/copper oxide nanoparticles: an update on their applications in biomedicine, mechanisms, and toxicity. <em>Biomolecules<\/em>, 11(4), 564. https:\/\/doi.org\/10.3390\/biom11040564<\/p>\n\n\n\n<p>[4]&nbsp;&nbsp;&nbsp;&nbsp; Siddiqi, K. S., &amp; Husen, A. (2020). Current status of plant metabolite-based fabrication of copper\/copper oxide nanoparticles and their applications: a review. <em>Biomaterials Research<\/em>, 24(1), 11.<\/p>\n\n\n\n<p>[5]&nbsp;&nbsp;&nbsp;&nbsp; Ashokkumar, M., Palanisamy, K., Ganesh Kumar, A., Muthusamy, C., &amp; Senthil Kumar, K. (2024). Green synthesis of silver and copper nanoparticles and their composites using <em>Ocimum sanctum<\/em> leaf extract displayed enhanced antibacterial, antioxidant and anticancer potentials. <em>Artificial Cells, Nanomedicine, and Biotechnology<\/em>, 52, 438\u2013448. https:\/\/doi.org\/10.1080\/21691401.2024.2399938<\/p>\n\n\n\n<p>[6]&nbsp;&nbsp;&nbsp;&nbsp; Abdulrasheed-Adeleke, T., &amp; Musa Bola, B. (2020). Comparative in vitro antioxidant activities of aqueous extracts of <em>Garcinia kola<\/em> and <em>Buchholzia coriacea<\/em> seeds. <em>Tanzania Journal of Science<\/em>, 46, 498\u2013507.<\/p>\n\n\n\n<p>[7]&nbsp;&nbsp;&nbsp;&nbsp; Imam, M. Z., Akter, S., Hoque Mazumder, M. E., &amp; Rana, S. (2011). Antioxidant activities of different parts of <em>Musa sapientum<\/em> L. ssp. <em>sylvestris<\/em> fruit. <em>Journal of Applied Pharmaceutical Science<\/em>, 1, 68\u201372.<\/p>\n\n\n\n<p>[8]&nbsp;&nbsp;&nbsp;&nbsp; Christenson, J. C., Korgenski, E. K., &amp; Relich, R. F. (2018). Laboratory diagnosis of infection due to bacteria, fungi, parasites, and rickettsiae. In <em>Principles and Practice of Pediatric Infectious Diseases<\/em> (5th ed., pp. 1422\u20131434.e3). Elsevier.<\/p>\n\n\n\n<p>[9]&nbsp;&nbsp;&nbsp;&nbsp; Khairy, T., Amin, D. H., Salama, H. M., Elkholy, I. M. A., Elnakib, M., Gebreel, H. M., \u2026 Sayed, H. A. E. (2024). Antibacterial activity of green synthesized copper oxide nanoparticles against multidrug-resistant bacteria. <em>Scientific Reports<\/em>, 14, 25020. https:\/\/doi.org\/10.1038\/s41598-024-75147-0.<\/p>\n\n\n\n<p>[10] Alok Kumar Srivastava, Virendra Kishor Sangode, K. V. Shalini, and Sangeetha Shanmugam (2026). Modern Nano-Fertilizer Delivery Systems and Nano-Biofertilizers: Advances, Mechanisms, and Sustainable Applications in Climate-Smart Agriculture: A Comprehensive Review. <em>Journal of Diversity Studies<\/em>. DOI: https:\/\/doi.org\/10.51470\/JOD.2026.5.1.146.<\/p>\n\n\n\n<p>[11] Rohan Gavankar, Deepa Verma, Ankita S. Tekade, and Virendra Sangode (2026). Green Synthesis and Characterization of Zinc Oxide Nanoparticles Using Cyperus pangorei Grass Extract and its Antibacterial Activity. <em>Journal of Diversity Studies<\/em>. DOI: https:\/\/doi.org\/10.51470\/JOD.2026.5.1.195<\/p>\n\n\n\n<p>[12]&nbsp; Kamal Vatika, Lisha, Shamal Kumbhar, Mehtab Yasmeen, Sunil Akare and Virendra K. Sangode (2024) Nanoparticle of Azadirachta indica (Neem) mitigating lead acetate induced reproductiive toxicity. Biochem. Cell. Arch. 24, 1101-1109. DOI: https:\/\/doi.org\/10.51470\/bca.2024.24.1.1101<\/p>\n\n\n\n<p>[13] Chetankumar B Masram, Virendra K Sangode, Prakash Tanji Wankhedkar, Manish Dnyaneshwar Baviskar, and Ravindra Yadav Bhandare [2026]. Green Synthesis of Silver Nanoparticles Using Murraya Koenigii: Characterization, Antioxidant, and Antibioilm Potential. <em>Journal of Diversity Studies<\/em>. DOI: https:\/\/doi.org\/10.51470\/JOD.2026.5.1.339<\/p>\n","protected":false},"excerpt":{"rendered":"<p>Introduction Metal oxide nanoparticles have attracted wide interest because their small size and large surface-to-volume ratio give them optical, catalytic and biological properties that differ from those of the bulk material. Among them, copper oxide (CuO) is a p-type semiconductor with a narrow band gap, and it is inexpensive and relatively easy to prepare [1,2]. [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"comment_status":"closed","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"ocean_front_end_style_editor":"no","ocean_post_layout":"","ocean_both_sidebars_style":"","ocean_both_sidebars_content_width":0,"ocean_both_sidebars_sidebars_width":0,"ocean_sidebar":"","ocean_second_sidebar":"","ocean_disable_margins":"enable","ocean_add_body_class":"","ocean_shortcode_before_top_bar":"","ocean_shortcode_after_top_bar":"","ocean_shortcode_before_header":"","ocean_shortcode_after_header":"","ocean_has_shortcode":"","ocean_shortcode_after_title":"","ocean_shortcode_before_footer_widgets":"","ocean_shortcode_after_footer_widgets":"","ocean_shortcode_before_footer_bottom":"","ocean_shortcode_after_footer_bottom":"","ocean_display_top_bar":"default","ocean_display_header":"default","ocean_header_style":"","ocean_center_header_left_menu":"","ocean_custom_header_template":"","ocean_custom_logo":0,"ocean_custom_retina_logo":0,"ocean_custom_logo_max_width":0,"ocean_custom_logo_tablet_max_width":0,"ocean_custom_logo_mobile_max_width":0,"ocean_custom_logo_max_height":0,"ocean_custom_logo_tablet_max_height":0,"ocean_custom_logo_mobile_max_height":0,"ocean_header_custom_menu":"","ocean_menu_typo_font_family":"","ocean_menu_typo_font_subset":"","ocean_menu_typo_font_size":0,"ocean_menu_typo_font_size_tablet":0,"ocean_menu_typo_font_size_mobile":0,"ocean_menu_typo_font_size_unit":"px","ocean_menu_typo_font_weight":"","ocean_menu_typo_font_weight_tablet":"","ocean_menu_typo_font_weight_mobile":"","ocean_menu_typo_transform":"","ocean_menu_typo_transform_tablet":"","ocean_menu_typo_transform_mobile":"","ocean_menu_typo_line_height":0,"ocean_menu_typo_line_height_tablet":0,"ocean_menu_typo_line_height_mobile":0,"ocean_menu_typo_line_height_unit":"","ocean_menu_typo_spacing":0,"ocean_menu_typo_spacing_tablet":0,"ocean_menu_typo_spacing_mobile":0,"ocean_menu_typo_spacing_unit":"","ocean_menu_link_color":"","ocean_menu_link_color_hover":"","ocean_menu_link_color_active":"","ocean_menu_link_background":"","ocean_menu_link_hover_background":"","ocean_menu_link_active_background":"","ocean_menu_social_links_bg":"","ocean_menu_social_hover_links_bg":"","ocean_menu_social_links_color":"","ocean_menu_social_hover_links_color":"","ocean_disable_title":"default","ocean_disable_heading":"default","ocean_post_title":"","ocean_post_subheading":"","ocean_post_title_style":"","ocean_post_title_background_color":"","ocean_post_title_background":0,"ocean_post_title_bg_image_position":"","ocean_post_title_bg_image_attachment":"","ocean_post_title_bg_image_repeat":"","ocean_post_title_bg_image_size":"","ocean_post_title_height":0,"ocean_post_title_bg_overlay":0.5,"ocean_post_title_bg_overlay_color":"","ocean_disable_breadcrumbs":"default","ocean_breadcrumbs_color":"","ocean_breadcrumbs_separator_color":"","ocean_breadcrumbs_links_color":"","ocean_breadcrumbs_links_hover_color":"","ocean_display_footer_widgets":"default","ocean_display_footer_bottom":"default","ocean_custom_footer_template":"","ocean_post_oembed":"","ocean_post_self_hosted_media":"","ocean_post_video_embed":"","ocean_link_format":"","ocean_link_format_target":"self","ocean_quote_format":"","ocean_quote_format_link":"post","ocean_gallery_link_images":"on","ocean_gallery_id":[],"footnotes":""},"categories":[24],"tags":[231,229,232,220,235,222,233,228,234,226,223,221,224,230,227,225,219],"article-archive":[196],"class_list":["post-838","post","type-post","status-publish","format-standard","hentry","category-original-research-article","tag-tulsi","tag-activity","tag-antibacterial","tag-antioxidant","tag-coli","tag-copper","tag-dpph","tag-escherichia","tag-ftir","tag-green","tag-nanoparticles-2","tag-ocimum","tag-oxide","tag-sanctum","tag-sem-edax","tag-synthesis","tag-xrd","article-archive-volume-6-issue-2-2026","entry"],"acf":[],"_links":{"self":[{"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/posts\/838","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/comments?post=838"}],"version-history":[{"count":1,"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/posts\/838\/revisions"}],"predecessor-version":[{"id":842,"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/posts\/838\/revisions\/842"}],"wp:attachment":[{"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/media?parent=838"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/categories?post=838"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/tags?post=838"},{"taxonomy":"article-archive","embeddable":true,"href":"https:\/\/academicsociety.org\/bio\/wp-json\/wp\/v2\/article-archive?post=838"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}